[mems-talk] Quartz wet etching

P.E.M. Kuijpers p.e.m.kuijpers at philips.com
Fri Dec 15 02:00:36 EST 2006


Dear Barbara,

Try to use a metal mask e.g. Cr.
After patterneing the Cr layer don't remove the resit befor BHF etching..

regards,
Peter Kuijpers
Philips


                                                                           
                                                                           
                                                                           
                                                                        To 
                                       "mems-talk" <mems-talk at memsnet.org> 
                                                                        cc 
     "Barbara Cortese"                                                     
     <KORTESEB at libero.it>                                          Subject 
                                       [mems-talk] Quartz wet etching      
     Sent by:                                               Classification 
     mems-talk-bounces at me                                                  
     msnet.org                                                             
                                                                           
     2006-12-14 05:10 PM                                                   
                                                                           
      Please respond to                                                    
         General MEMS                                                      
          discussion                                                       
     <mems-talk at memsnet.o                                                  
             rg>                                                           
                                                                           
                                                                           




Dear all
I'm wet etching quartz with a BHF solution 6:1, but I have encounterd some
difficulties in etching.
What I do is a photolithographic process on the quartz substrate, a
hardbake of 4 hours at 180° and then the wet etching process.
What I obtain though is the rearrangement of the photoresist in a
disordered pattern and no etching!
Has anyone an idea where I go wrong?
Barbara
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk




More information about the MEMS-talk mailing list