[mems-talk] Thick SiO2 etch
P.E.M. Kuijpers
p.e.m.kuijpers at philips.com
Fri Apr 20 02:01:12 EDT 2007
Dear Xiaoguang "Leo" Liu,
A solution can be to use also a structured Cr mask below you resist
before etching the SiO2 layer.
We found that this gives better resulst than only a resist mask.
Regards,
Peter Kuijpers
MiPlaza
DTS/TFF
Phone.: (+31 40 27) 98904 (mobex)
mobile:(+31) 06-12507027
fax.: [+31 40 27) 44769
mailto:p.e.m.kuijpers at philips.com
"Xiaoguang \"Leo\" Liu" <liuxiaoguang at gmail.com>
Subject [mems-talk] Thick SiO2 etch Classification
Dear all
For one of my projects, I need to pattern thick thermal oxide of
1.5um. I used 49%HF:DI = 1:6 as the etchant and 20um AZ9260 as a mask
(the reason of using this thick resist is that I need to do a through
wafer Deep RIE after patterning the SiO2).
The etching of the oxide takes more than half an hour in the etchant.
My problem is that the photoresist can not stand the HF solution and
start to peel off (especially the smaller features) after about 20min.
HF also attacks the photoresist reducing the overall thickness of the
photoresist, which can impact my later DRIE process.
Could anybody illuminate me with a better method to etch the oxide
layer without destroying the photoresist?