[mems-talk] photoresist suggestion

Cain, Mike Mike.Cain at MEMSCAPINC.COM
Thu Aug 16 10:14:00 EDT 2007


Hello Andrea,

Your lithography process sounds fine.  Shipley makes S1827 positive photoresist that is designed for thicker coat applications.  The "peeling" you describe may be the resist is being undercut so thicker (or different) resist may not help.

Good Luck,

Mike

-----Original Message-----
From: mems-talk-bounces at memsnet.org [mailto:mems-talk-bounces at memsnet.org] On Behalf Of Andrea Mazzolari
Sent: Wednesday, August 15, 2007 6:19 PM
To: guitiz at bu.edu; General MEMS discussion
Subject: [mems-talk] photoresist suggestion


Hi all, i need to pattern a 400um thick silicon nitride film. I'm planning to use BHF (1:7) to remove silicon nitride from unwanted areas. Etch rate of silicon nitride is about 1nm/min, so the etch time will be about 400 min. About photoresist: i've tried to use s1813, but it peel off after about 5 hours etch.

Here is the procedure i've followed:
spinning of primer
spinning of s1813
soft bake (2 min at 120 °C)
photolitography
hard bake (2 min at 120 °C)

How can i improve s1813 resistance to BHF? May a thicker s1813 layer help ? Or a longer hard bake time ? Any idea about an alternative photoresist ?


More information about the MEMS-talk mailing list