[mems-talk] How to uniformly etch ~0.05 - 0.3um off a 3" Si wafer?

Kirt Williams kirt_williams at sbcglobal.net
Fri Dec 21 14:23:06 EST 2007


A trick I've seen used to remove surface damage from grinding and polishing 
is to grow a thermal oxide, then etch it off in an HF solution, say 5:1 BHF.
It's standard practice to perform a nitrogen anneal after oxidiation to 
recover some of the damage caused by oxide growth.
The silicon thickness used to grow oxide is 46% of the oxide thickness; for 
example, a 0.22-um oxide consumes 0.1 um of silicon.
    --Kirt Williams

----- Original Message ----- 
From: "Dave Goldstein" <d.goldstein.2007 at gmail.com>
To: <mazzolari at fe.infn.it>; "General MEMS discussion" 
<mems-talk at memsnet.org>
Sent: Wednesday, December 19, 2007 7:21 PM
Subject: Re: [mems-talk] How to uniformly etch ~0.05 - 0.3um off a 3" Si 
wafer?


> Thanks Edward and Andrea for the reply!
> I need to remove the top ~ 0.1 um of Si with diffusion 'cause I am
> suspecting my top surface is rich with defects due to the saturating
> concentration of dopants right at the surface.
>
> About surface roughness: I think you don't get rougher than 0.1um when you
> are etching 0.1um off. And my requirement for surface roughness is very
> lenient. 0.1um will do. But uniformity is the problem.
>
> I have a small RIE (Plastherm 790) but it doesn't give me much uniformity
> over 3" wafer.
>
> right now I am thinking about using low temperature UV oxidation to create
> some oxide and then remove them by HF.
>
> More suggestions?
>
> On Dec 19, 2007 12:57 PM, Andrea Mazzolari <mazzolari at fe.infn.it> wrote:
>
>> Hello Dave,
>> which is the thickness you need to remove ? Which is wafer orientation ?
>> Which is surface rougness you can accept ?