Dear Arti,

I normally use Al for masking in the ICP by Al evaporation. I can etch
through-hole of a 500um wafer with around 300nm evaporated Al layer. Al can
be evaporated well to SiO2 as well. I don't know if you can use Al or you
have to use photoresist.

Regards,
Nam LE

On 6/29/07, Bill Moffat <BMoffat at yieldengineering.com> wrote:
>
> Isaac is nearly right.  The trick is to stop any chance of moisture
> before the HMDS is applied.  Easiest way is vacuum/hot Nitrogen
> dehydration followed by HMDS vapor while the product is still in a
> vacuum dehydration chamber.
> Bill Moffat, CEO
> Yield Engineering Systems, Inc.
> 203-A Lawrence Drive, Livermore, CA  94551-5152
> (925) 373-8353
>
> bmoffat at yieldengineering.com
>
> www.yieldengineering.com
>
>
> -----Original Message-----
> From: mems-talk-bounces at memsnet.org
> [mailto:mems-talk-bounces at memsnet.org] On Behalf Of Isaac Chan
> Sent: Thursday, June 28, 2007 7:57 AM
> To: Arti Tibrewala; General MEMS discussion
> Subject: Re: [mems-talk] Re: Mask for ICP (dry etching)
>
> Arti,
>
> Can you do a quick bake above 100C then cool it down with N2 gun and
> spin coat HMDS immediately?
>
> Isaac
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>


More information about the MEMS-talk mailing list