[mems-talk] Adhesion layer for Nickel during Liftoff process

David Nemeth nemeth at sophiawireless.com
Mon May 14 08:50:35 EDT 2007


I don't know what surface you had on before the Ti, but adhesion layers work
best if they are prepared in-situ.

In other words, try first putting down the PMMA, then put down the Ti and
the Nickel during the same pumpdown.  

David Nemeth

-----Original Message-----
From: mems-talk-bounces at memsnet.org [mailto:mems-talk-bounces at memsnet.org]
On Behalf Of madhav rao
Sent: Friday, May 11, 2007 8:31 PM
To: mems-talk at memsnet.org
Subject: [mems-talk] Adhesion layer for Nickel during Liftoff process

Hi All,
       I had sputtered Titanium layer. then I did spin
oat of PMMA. After exposing it (E-beam lithography),
Nickel was deposited using E-beam evaporation. Finally
Liftoff was carried out to remove PMMA. However after
liftoff, I could not see any Nickel and Titanium.
Please let me know, which is the better adhesive metal
for Nickel in Liftoff process.


More information about the MEMS-talk mailing list