[mems-talk] Another question about silicon dioxide wet etching

Kirt Williams kirt_williams at sbcglobal.net
Mon Nov 19 12:16:51 EST 2007


For the question "Can the fabrication method of SiO2 make such a big 
difference in etching rate?" the answer is "yes, it can make an enormous 
difference."
Some methods of obtaining a layer of SiO2 are sputtering, thermal growth, , 
LPCVD with annealing, LPCVD without annealing, and PECVD.
These are listed in order of slowest-etching to fastest etching.
In addition to deposition method, the addition of other oxides such as 
phosphorous oxide (as in PSG) or boron oxide (as in BSG) can increase or 
decrease the etch rate.
Annealing (e.g., at 1000 C for 1 hour) can decrease the etch rate of CVD 
oxides.
For tables of hundreds of measured etch rates, along with documentation of 
preparation methods, see two papers from JMEMS:
http://microlab.berkeley.edu/labmanual/chap1/JMEMSEtchRates1(1996).pdf
http://microlab.berkeley.edu/labmanual/chap1/JMEMSEtchRates2(2003).pdf
    --Kirt Williams

----- Original Message ----- 
From: "Xiaoning Wang" <wxn0000 at gmail.com>
To: <mems-talk at memsnet.org>
Sent: Saturday, November 17, 2007 9:36 AM
Subject: [mems-talk] Another question about silicon dioxide wet etching


> Hello everyone!
>
> I am a undergraduate student in Peking University, China.
>
> I have been doing some experiments on silicon dioxide sacrificial layer
> etching lately. And I used 4 parts NH4F (40%), 2 parts glycerin and 1 part
> HF(40%) as the etchant. I noticed that the etching rate of silicon dioxide
> was about 5000A/min at room temperature, far above those rates reported in
> literatures even without heating. Can the fabrication method of SiO2 make
> such a big difference in etching rate? Or is there any other possible
> explanations for that?
>
> Also, I found that Aluminum's etching rate was lower when the etchant
> solution's temperature increased. Does that make any sense? Since normally
> the etching rate should go up when heated, right? I tried to explain this
> from a chemical kinetics' point of view, but was limited because of my 
> major
> (electrical engineering). So was that I screwed up my experiments? (though 
> I
> hope it's not likely) Or would anyone can tell me the reason, please?
>
> Thank you for your time!
>
> Best wishes!
>
> btw, are there any differences between glycerin and glycerol? Their 
> Chinese meanings are exactly the same.
>


More information about the MEMS-talk mailing list