[mems-talk] Thin Film problem

Yeswanth Rao yrao at engr.uga.edu
Tue Nov 27 16:08:46 EST 2007


I have been depositing thin metallic films on glass substrate using an E-beam evaporator in the following order:

Ti(15nm)/Cu(200nm)/Al(1.2micron) - After deposition, I anodize the aluminum layer and during anodization at constant potential the current is 2mA - This process works fine!

But, when I use the following sample: Ti(15nm)/Au(200nm)/Al(1.2micron) and after e-beam deposition, when I anodize the film at constant potential, the current is 100-140mA which is unusually high. After anodizing for a couple of minutes, the aluminum lays just dissolves away. 

Does anyone have any suggestions as to why this may be happening. Is the problem associated with the deposition of these metallic layers or something else? Any information or suggestions will be very helpful

Yeswanth L Rao
UGA
Athens, GA


More information about the MEMS-talk mailing list