Dear Steve,

If it will work with your process, you might want to try the SU-8 3000 series. The aspect ratios you can achieve with it aren't as good, but it does have improved adhesion on ITO.

The datasheet is here:
http://www.microchem.com/products/pdf/SU-8%203000%20Data%20Sheet.pdf

Alternatively, you could use an adhesion layer. For pillars, this would work by patterning something SU-8 adheres well to (such as Ta) on the ITO.

If you're doing SU-8 pillars on ITO, I'm guessing it's for some sort of surface with switchable hydrophobicity. If this is the case, that Ta pad shouldn't make much of a difference.

Finally, omnicoat might work, but I'm not sure what the chemistry would be at an ITO surface. It's worth looking at though, at least.

- Kevin

*********************************
Kevin Paul Nichols
PhD Student
MESA+ Institute for Nanotechnology
Mesoscale Chemical Systems
Meander 151
University of Twente
Postbus 217
7500 AE Enschede
The Netherlands

Office: +31 (0)53 489 26 31
Mobile: +31 (0)6 49 312 471
Fax   : +31 (0)53 489 35 95
Email : k.p.nichols at utwente.nl

-----Original Message-----
From: mems-talk-bounces at memsnet.org on behalf of Steve Jung
Sent: Tue 9/11/2007 8:20 AM
To: mems-talk at memsnet.org
Subject: [mems-talk] SU-8 adhesion on ITO coated glass
 

Dear all,


I am planning to build SU-8 pillars for a microfluidic device
but have some questions in choosing the right product.

The SU-8 pillars (ca. 10um) are supposed to be built on
an ITO coated glass and I heard the adhesion of SU-8 on
glass substrate is very poor. 


Does the adhesion property get worse on ITO coated glass 
substrates than on normal glass substrates?


Also, does the adhesion property of SU-8 2000 (MCC)
differ from the original SU-8 (MCC)?

If so, could anyone tell me which product would more
be advantageous to coat on an ITO coated glass substrate?