Cr and gold mix at temperatures >150c so you should try Ti or TiW.
Rick
-----Original Message-----
From: mems-talk-bounces at memsnet.org [mailto:mems-talk-bounces at memsnet.org] On Behalf Of Heiko Prüßner
Sent: Thursday, April 03, 2008 5:42 AM
To: General MEMS discussion
Subject: [mems-talk] Hf resistant Adhesion layer for Au on Si
Dear all,
I had a 20nmCr/ 200nmAu film sputtert on silicon. This setup has been treated at 350°C for an hour. At the final Hf etching step which I used to remove the BOX of an SOI wafer the Au film peeled of.
Does anybody have an explanation? Do I need a diffusion barrier between the Cr and the Au? Or has anyone a suggestion for another adhesion layer?