> I am experiencing a problem in patterning on silicon-di-oxide wafers; I am using SHIPLEY 1818 resist to get a thickness of 2.5 micron; 6 seconds of exposure time. After developing for 60 seconds, I observe, the resist layer peels off; leaving no patterns on the wafer. Also I had soft-baked the resist at 95 C for 2 minutes in hot-plate.
> This seems strange to me, as a month ago, I had successfully transferred the patterns on to silicon-di-oxide wafers.
> I am using mylar film masks.
> Please let me know, if any one had experienced similar problems before; and if so, could you let me know suggestions to solve ?
> Madhav Rao,
> Graduate student,
> University of Alabama.
Madhav,
1. exposure time without the context of the uv light intensity is
meaningless. You might want to borrow a uv light meter and see how
much the lamp has dimmed in the intervening months. Nevertheless S1818
is a positive resist and only the areas exposed to UV should be
developing away.
2. you mentioned you performed this procedure several months ago:
Assuming nothing has changed, may I suggest a pre-spin bake of your
substrate on a 120 C hot plate or oven to improve resist adhesion. Let
the substrate cool before you spin, but in a dry place (nitrogen?) If
your substrates are subject to humid air (summer in alabama) it may be
reducing adhesion. You might also try an adhesion promoter.
Regards,
Jon Fox
Dr. Jon R. Fox
email: drjonfox at gmail.com
website: http://www.drfox.com
facebook: http://www.facebook.com/profile.php?id=536676463
linkedin: http://www.linkedin.com/in/drjonfox
More information about the MEMS-talk
mailing list