[mems-talk] SU8 Processing
Sexton Mike
M.Sexton at EVGroup.com
Tue Mar 25 11:29:21 EST 2008
I have done similar processes and was able to get roughly 250um on a
single spin. My spin speed was about the same as yours. My suggestion
would be to decrease your spin time. With the thicker resist spin time
has a dramatic effect on film thickness. I would try a spin time of
40-60 seconds. This was done on 8" substrates so there may be some
adjustments to spin speeds and time. Having the relax step to even out
the surface is also a very good step to improving your uniformity.
In addition I'm not sure what effect it will have but the recommended
developer for SU8 is PGMEA, not Acetone.
Best Regards,
Mike Sexton
EV Group
invent * innovate * implement
Process Technology Engineer - Direct: +1 (480) 305 2450, Main: +1 (480)
305 2400 Fax: +1 (480) 305 2401
Cell: +1 (602) 625 1275
E-Mail: M.Sexton at EVGroup.com, Web: www.EVGroup.com
-----Original Message-----
From: mems-talk-bounces at memsnet.org
[mailto:mems-talk-bounces at memsnet.org] On Behalf Of Owen The
Sent: Sunday, March 23, 2008 10:16 PM
To: mems-talk at memsnet.org
Subject: [mems-talk] SU8 Processing
Hi all, I've been having some trouble with my SU8 Processing.
Currently I'm using SU8 2100. I'm trying to get a postbaked thickness
of 260um, but I've been consistently getting half the quoted thickness
(130um in this case) for any given speed.
Here's my processing steps:
1) Wafer prep
2) Dispense 4ml of SU8 on a slowly spinning wafer (to center the blob)
3) Ramp to the set speed (in this case 1000 RPM), hold for a few minutes
and then stop
4) Rest in a covered petri dish on top of a small filter with a little
acetone (to even out the surface)
5) Softbake (ramping to set temps)
6) Expose and postbake (ramps to temps again)
7) Develop in acetone, rinse with isopropanol and water
Not sure what I'm missing, but I've done this process with other
grades of SU8 and have always seen 50% of the quoted film thickness.