A recipe I've used for PECVD SiN on a Pacific Western Systems Coyote is: 330 sccm SiH4 (100%) 2000 sccm NH3 300 watts RF Power pressure = 2 torr Roger Shile ----- Original Message ----- From: "Dlee Li"To: Sent: Friday, June 20, 2003 2:17 PM Subject: [mems-talk] PECVD Si3N4 recipe > Hi, > anyone can give me his workable PECVD Si3N4 recipe? we need to add PECVD > Si3N4 to our system. > > thanks > Dlee > > _________________________________________________________________ > MSN 8 helps eliminate e-mail viruses. Get 2 months FREE*. > http://join.msn.com/?page=features/virus > > > _______________________________________________ > MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list > options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk > Hosted by the MEMS Exchange, providers of MEMS processing services. > Visit us at http://www.memsnet.org/