Hi, You can try 10% HF or I like to use 98% H2O2/2% NH4OH. Rick -----Original Message----- From: mems-talk-bounces+rmorrison=radantmems.com@memsnet.org [mailto:mems-talk-bounces+rmorrison=radantmems.com@memsnet.org]On Behalf Of kris Sent: Tuesday, July 01, 2003 11:49 AM To: General MEMS discussion Subject: [mems-talk] Ti Etch Dear all, I am trying to etch Ti(300 Angs),which has aluminum layer underneath it.I have used TiW-30 (25-40C)from transene.I could see that after some time the Ti etch rate reduces completely and etch almost stops.I think due to the formation of Tio2 the etch rate drops. Can anyone suggest me a good Titanium etchant that should not attack Al. Your suggestions are highly helpful. Thanks Kris __________________________________ Do you Yahoo!? SBC Yahoo! DSL - Now only $29.95 per month! http://sbc.yahoo.com _______________________________________________ MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk Hosted by the MEMS Exchange, providers of MEMS processing services. Visit us at http://www.memsnet.org/