Hi Nishant, There are a number of techniques you can use to reduce or circumvent stiction problems 1) supercritical CO2 drying after wet release. I dont know much about this since it was done for me, but seemed to be successful every time. 2) If you don't have the tool for supercritical CO2, try dipping your samples in hexanes right after the wet release (3 baths: etch, dip in H2O and dip in hexanes, keeping the samples wet as you transfer from bath to bath) and let them dry as you pull them slowly out of the hexanes. Good luck Jobert vanm Eisden SUNY Albany -----Original Message----- From: Saurabh Nishant [mailto:nishu7uf@yahoo.com] Sent: Friday, October 24, 2003 7:16 AM To: mems-talk@memsnet.org Subject: [mems-talk] polysilicon stiction problem Dear MEMS colleagues, I am a student at indian institute of science and facing the problem of stiction in polysilicon cantilivers after sacrificial layer etching.I would appreciate if any one can suggest me some means to overcome this problem.I suspect both the resifual stress and capillary forces are reponsible.Any help would be highly appreciated. thanks. regards nishant --------------------------------- Do you Yahoo!? The New Yahoo! Shopping - with improved product search _______________________________________________ MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk Hosted by the MEMS Exchange, providers of MEMS processing services. Visit us at http://www.memsnet.org/