Stephan You can try the reflow technique where you first sputter deposit 300-500nm Ti wetting layer, and then sputter deposit the Aluminum at a very low dep rate and substrate temp in the range of 450-500C. Best of luck. With regards, (Pramod Gupta) Stephan Biberwrote: Dear MEMS group! We machine trenches with about 200um depth into a silicon wafer. The trench width is about 30-50um yielding an aspect ratio of 1:4 to 1:7. We want to plate the whole structure with a highly conductive metal such as Gold, Platinum, Copper, Aluminum or Silver. We need the trenches to be completely covered with at least 200nm of metal. 1. Is it possible to do that by sputtering, despite the high aspect ratio? 2. Does anyone know a method how to do that? E.g. electroless plating? 3. Does anyone have experience with such a problem? Any hints will be greatly appreciated! Stephan -- _______________________________________________ MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk Hosted by the MEMS Exchange, providers of MEMS processing services. Visit us at http://www.memsnet.org/ (Pramod Gupta) 20800 Valley Green Dr., # 445 Cupertino, CA 95014 Phone: (408) 253-1646 --------------------------------- Do you Yahoo!? Free Pop-Up Blocker - Get it now