Dear Dave,
Thanks for your reply but sir, I also want to know about the
solution making procedure because last time I just mixed the KI and I2 powders
and made the solution with DI water, which is not the correct way of making the
solution because Iodine is very volatile.
Hare Krishna
aasutosh dave wrote:
Hare Krishna,
I use 20gm KI : 5gm Iodine : 160 ml DI water. You can change the
concentration too to achieve higher etch rates. If you want you can reuse it
for few times but not more as you will notice the etch rate will change each
time you resue it. As far as I know you can preserve in any sealed glass or
plastic bottle.
Regards,
Aasutosh Dave
Nanofab Center
Arlington, Texas
>From: hare krishna
>Reply-To: General MEMS discussion
>To: mems-talk@memsnet.org
>Subject: [mems-talk] Preparation of KI+I2+DIwater solution for gold etching
>Date: Sun, 8 Feb 2004 05:47:03 +0000 (GMT)
>
>
>Dear All,
> How should I make the solution of KI + I2 + DI water for the
>gold etching. Should I use it fresh or I can use it for long time...and how
>should it be preserved.
>Regards
>Hare Krishna
>
>
>
>Yahoo! India Education Special: Study in the UK now.
>_______________________________________________
>MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list
>options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>Hosted by the MEMS Exchange, providers of MEMS processing services.
>Visit us at http://www.memsnet.org/
_________________________________________________________________
Let the advanced features & services of MSN Internet Software maximize your
online time. http://click.atdmt.com/AVE/go/onm00200363ave/direct/01/
_______________________________________________
MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/
Yahoo! India Education Special: Study in the UK now.