As with oxide etching, etching nitride with selectivity to silicon is usually done by depositing fluorocarbon polymer on the wafer. Suitable gases to deposit such a polymer are CHF3, C4F8, or more generally C_xF_yH_z where (y-z)<=2x (which maximises the density of CF2 radicals in the plasma) The etchants (F) have to diffuse through this polymer film to attack the substrate, so etch rate is very sensitive to film thickness. Reaction with the nitrogen in the film reduces the polymer thickness, so the nitride etches faster than the silicon, despite its stronger chemical bonding. See Schaepkens etc al, JVST A 17, 29 (1999) for a very clear experimental study. Regards, Nick Dr Nick Appleyard Research Physicist Etch Product Group, Trikon Technologies Ltd Ringland Way, Newport, South Wales, NP18 2TA Tel (44) 01633 414187 Fax (44) 01633 414180 Mob (44) 0788 178 0727 Dear all: I would like to find out a RIE recipe which performs a selective etching between nitride and silicon. I only know that CHF3 is one of the suitable etching gas. Does anybody know the recipe, including gas types, flow rate, power, pressure, and etching rate? The RIE facility here only provides SF6, CF4, O2, N2, CHF3, etc. The max power is 300W. Please give me some advice if possible. I really appreciate it. Yi Chun Dept. of Power Mechanical Engineering, National Tsing Hua University, Taiwan. ======================================================= This communication is for the sole use of the intended recipient(s)and may contain confidential and privileged information. Any unauthorized review, use, disclosure or distribution is prohibited. If you are not the intended recipient, please contact the sender by reply email and destroy all copies of the original message. To reply to our email administrator directly, send an email to postmaster@trikon.com TRIKON TECHNOLOGIES - Manufacturers and suppliers of PVD, CVD and Etch equipment for the semiconductor and related industries. http://www.trikon.com ======================================================= This message has been checked for all known viruses by Star Internet delivered through the MessageLabs Virus Scanning Service.