Jeff Babinski
2004-09-09
Do you happen to be using an i-line filter?  A broadband exposure tends to
cause features to be less defined using SU-8 as you have described, making
use of a 365nm i-line filter necessary.

Jeff Babinski
Process Engineer
Microfabrication Solutions

-----Original Message-----
From: mems-talk-bounces@memsnet.org
[mailto:mems-talk-bounces@memsnet.org]On Behalf Of suscarl
Sent: Wednesday, September 08, 2004 11:15 AM
To: mems-talk@memsnet.org
Subject: [mems-talk] unwanted tapering of SU-8 structures


Need advice from SU-8 experts:
I have 30um width by 55um height SU-8 2035 lines. Somehow, after 35s
exposure time and post-bake of 95oC for 20min, the resulting structures are
tapered with bottom 60um width and top 40um width. Can anyone offer possible
solutions to troubleshoot the problem?

Thanks!!
_______________________________________________
MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply