We've used diluted NaOH at room temperature. The etch is rather slow, but if it's heated it will start to etch the ITO as well. AZ 300 developer also works rather well. There are also commercial etchants available selective to ITO. -Jeff Campbell Eugenie Shelegeda wrote: >Dear all. > >Does anyone know an ITO wet/dry etchant which is selective to Al. > >Does anyone know more wet ITO etchants. >I know only these:( > >1HCl : 1H2O, rate = 0.8 nm/sec >1HF : 1H2O2 : 10H2O, rate = 12.5 nm/sec > >Best regards, >Eugenie Shelegeda. > >_______________________________________________ >MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list >options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk >Hosted by the MEMS Exchange, providers of MEMS processing services. >Visit us at http://www.memsnet.org/ > > >