Dear Karin,
If thermal contact is d main issue in etch rate variation, then you
can try Spin coat 'Photoresist' on your 3"Carrier wafer and nicely place
all your waferpieces. After that do a normal hardbake recommended for
the photoresist which you are using. You might know well how to remove
the resist, 'acetone' will do it nicely. I got good consistency in etch
rate and profile by doing this way, moreover I found this way is more
comfortable in fixing and removing the samples from the carrier wafers.
Good Luck
Mohanraj
Karin Buchholz wrote:
> Dear mems talkers,
>
> we have a RIE chamber with temperature control of the 3" carrier
> wafer. Since we are just using waferpieces we just place these on top
> of the carrier wafer. It seems now that these small pieces
> do not have proper thermal contact to the chuck, so the temperature
of
> the sample is not constant
> from etch to etch and the etch rate also varies by 50per cent...
>
> Do you have any suggestions how to provide good thermal contact? The
> manufacturer suggested Fomblin vaccuum oil, but it is impossible to
> remove it from the samples after etching...
>
> I appreciate any help! Have a nice day,
>
> Karin
>
> --
> Dipl.-Ing. Karin Buchholz
> Walter Schottky Institut
> Technische Universitaet Muenchen
>
> _______________________________________________
> MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list
> options, visit
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
begin:vcard
n:Garber;R. Brent
tel;fax:(860) 486-3756
tel;work:(860) 486-6679
x-mozilla-html:TRUE
org:University of Connecticut;Optoelectronic Science Center version:2.1
email;internet:garber@engr.uconn.edu
title:Sr. Research Specialist adr;quoted-printable:;;UCONN=0D=0A54 Ahern
Lane=0D=0AU-5219;Storrs;CT.;06269;
fn:R. Brent Garber
end:vcard
********************************************************************************
***
This email and any files transmitted with it are confidential and intended
solely for the use of the individual or entity to whom they are addressed. If
you have received this email in error please notify the system administrator.
********************************************************************************
***