I need more information. If you are trying to bond a flexible polyurethane film to glass, plasma bonding is easy. I have used plasma times as low as 10 seconds and got terrific unpeelable bonds. the secret is the uniformity of the plasma, and both surfaces need plasma treatment together. The polyurethane needs the short time, with longer times it gets too hot. The glass can withstand much longer time and if I was trying to bond glass to glass I would use times like 5 minutes. Bill Moffat