durusmail: mems-talk: PDMS bonding to glass
PDMS adhesion
2005-05-30
2005-05-31
PDMS bonding to glass
2005-06-01
2005-06-01
2005-06-01
PDMS bonding to glass
Lee Pang
2005-06-01
You can acid treat the PDMS surface.  I've typically placed PDMS blocks
in warm 0.1N HCl for 2hrs and then heat cured the blocks onto glass at
80degC overnight.  This will give you a good bond, but it won't be
irreversible - e.g. a fully enclosed 1 x 1mm feature can only withstand
about 8-10psi of applied pressure before bursting.

Lee Pang
wpang@ucsd.edu


-----Original Message-----
From: Kamat Mahesh Keshav
Subject: [mems-talk] PDMS bonding to glass

Is it possible to bond PDMS to glass without using oxygen plasma method?
I mean ...is there another alternative?