This could definitely work, especially depending on the time between exposure and develop. As soon as the SU-8 is exposed, it begins crosslinking, but at room temperature, this crosslinking occurs slowly. Its possible that enough crosslink occurred to allow development with reasonable fidelity, without crosslinking beyond the point of ashability. I've done processes similar to this myself. Based on my observations, SU-8 crosslinking is a catalyzed process - once the photo-acid is present (in any quantity), it will begin the cross-link process. Concentration of acid (controlled by exposure dose) influences rate of reaction, as does temperature (as in most chemical reactions, heat accelerates the process). By reducing the concentration of the acid (reduced exposure), and reducing reaction kinetics (lower temp bake), I've been able to crosslink SU-8 sufficiently to pattern it (at >100 µm thick, and maintaining near 90º sidewalls), while still being able to bond the material via standard thermocompression bonding (which requires some degree of reflow in the SU-8). Best Regards, Chad Brubaker EV Group invent * innovate * implement Senior Process Technology Engineer - Direct: +1 (480) 305 2414, Main: +1 (480) 305 2400 Fax: +1 (480) 305 2401 Cell: +1 (602) 321 6071 E-Mail: C.Brubaker@EVGroup.com, Web: www.EVGroup.com -----Original Message----- From: mems-talk-bounces@memsnet.org [mailto:mems-talk-bounces@memsnet.org] On Behalf Of Bob Henderson Sent: Tuesday, September 15, 2009 1:23 PM To: 'General MEMS discussion' Subject: Re: [mems-talk] SU8 James: This has been a long time ago but if I remember right we treated it just like negative working resist. That is we had a special SU8 that would produce a 5 micron film at 3,000 rpm spin speed. After coat we did a soft bake at 70 degrees C for 30 minutes in a Blue M oven. Then we exposed on a contact aligner to cross-link the exposed areas with proper wavelength of light. Then we developed using Xylene followed by N-Butyl Acetate for a rinse. The sidewall profile was 90 degrees and it had much better selectivity to a silicon etch than any positive resist we tried. That is all I remember but you can contact MicroChem as I am sure they have advanced the formulations since then. Bob Henderson