Dear Chakry, pH is a good indicator for aluminum passivatoin in doped TMAH. You have to keep the pH at 12. If the pH is higher than 12, such as 12.3, you can literally see the aluminum disappearing. If the pH is lower than 12, the etching rate of silicon is decreased. You can find this information from many articles about TMAH. You might need to put more chemical that you are currently using in order to drop the pH. Some of your descriptions are not clear to me. Would you describe more in detail about your recipe? What does "40% SA aqueous solution" mean? Is this silicic acid? Also, how did you make 40% SA solution? Would you tell me how many gram of what chemical you put in a liter of water or TMAH solution? What is the resource for this recipe? Is there any specific reason for using 10% TMAH solution? I cannot tell much about it based on your description. __________________________________________________________ Il-seok Son (Sunny) Dept. of Electrical and Computer Engineering University of Wisconsin - Madison, SonicMEMS __________________________________________________________ ----- Original Message ----- From: "chakravarthy.S.Yamarthy"To: Sent: Sunday, May 26, 2002 3:57 PM Subject: [mems-talk] TMAH Etching > Dear friends, > > i am trying to do TMAH etching of silicon under the > cantilever beam made of (silicon > dioxide+polysilicon). > > We have used the solution of TMAH(10% w/w in > water)+SA(40% aqueous solution)+Ammonium peroxy > disulphate(APODS about 1.25gms). > > we have heated the entire solution @ 80 degree > centigrade and chips were etched in this solution. > > But,we could see that Al bond pads,which were opened > thru silicon dioxide passivation layer(9000 Angs)were > attacked by the etching solution. > > Can anyone of u please suggest me any good etching > technique for silicon that should not attack Aluminum. > > thanks > Chakry > > ===== > To Know That We Know What We Know,And That We Do Not Know,What We Do Not > Know:That Is The True Knowledge. > Confucius > Yahoo! - Official partner of 2002 FIFA World Cup > http://fifaworldcup.yahoo.com > _______________________________________________ > mems-talk@memsnet.org mailing list: to unsubscribe or change your list > options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk > Hosted by the MEMS Exchange, providers of MEMS processing services. > Visit us at http://www.mems-exchange.org/