Dear Bo We sonicate in acetone for about 15min, followed by piranha, followed by HF. That seems to do the trick on the Si masters. Chris On Wednesday, November 20, 2002, at 08:51 PM, bhe063@lulu.it.northwestern.edu wrote: > I got a problem when peel off PDMS off the Si mold made by > DRIE since I > did not treat the mold before pour PDMS on. After that, I tried to use > HF to > remove PDMS so that I can use the mold again. But it takes very long > and the > cleaning is not complete. Can anybody give some suggestions how to > totally > remove the PDMS from the Si mold? Any input is highly appreciated. -- Christopher F. Blanford Inorganic Chemistry Laboratory, South Parks Road, Oxford, OX1 3QR, UK Phone: (44)/(0)-1865-282603; Fax: (44)/(0)-1865-272690 PGP keyID: 8D830BC9 http://pgp.mit.edu/