I have anodically bonded Pyrex to silicon wafers with several thousand Angstroms of oxide. I've also anodically bonded Pyrex to a 6000 Angstroms film of Silicon Nitride. Before bonding to the nitride it must be "annealed" in wet oxygen at 1100 degC for 4 hours (sounds like oxidation to me). The bonding, is then done for 4 hours at 400 degC with -400 volts applied to the Pyrex. My understanding is that the surface to which the Pyrex is bonded must be oxidized. Pyrex or other glass containing mobile ions can be anodically bonded to silicon or to metals that oxidize, such as Al, but not to metals that don;t oxidize such as Au. Roger Shile ----- Original Message ----- From: "Hell, Erwin"To: Sent: Monday, March 17, 2003 6:20 AM Subject: [mems-talk] dielectric layer > Hi all, > does anyone has experience/knowledge about anodic bonding with a dielectric > layer between glass and silicon? How does it affect the bond quality? > > Any recommendations are appreciated > > ------------------------------------------------------------------ > SUSS MicroTec > Hell Erwin > Product Specialist > Aligner & Bond Systems > Schleissheimerstr.90 > D-85748 Garching > Germany > ********************************** > Tel. +49 (0) 89 32007 307 > Fax. +49 (0) 89 32007 162 > Cell: +49 (0) 170 5386531 > Email: hell@suss.de > Int: http://www.suss.com > > _______________________________________________ > MEMS-talk@memsnet.org mailing list: to unsubscribe or change your list > options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk > Hosted by the MEMS Exchange, providers of MEMS processing services. > Visit us at http://www.memsnet.org/