What do you mean by no success - poor quality or something else? The type of glass is also relevant. I have had good results with 2% conc. HF + 2% conc. HNO3 when using soda-lime glass. I have never tried it on quartz though, but I would not expect it to etch at a similar rate. Barbara Cortese wrote: > Hi to all > > I'm etching glass and quartz by a wet etching solution of BHF, but my recipe isn't too good. I've tried differrent solutions with no success. Has anyone a good recipe to suggest me?(not just saying BHF 6:1! but the effective quantities!). > >