Questions regarding HMDS (Hexamethyldisilazane)
Nathan McCorkle
2013-12-20
How does FDTS compare to HMDS?

On Tue, Dec 17, 2013 at 2:32 PM, Bill Moffat
 wrote:
>
> Daniel, good question.  Here is my experience.  First the problems with resist
adhesion are usually caused by moisture and as the three vacuum purges with hot
nitrogen between the vacuum purges absolutely dehydrate the wafers, which is a
great start.  The HMDS molecule bonds to the wafer surface replacing the H in
the Hydroxyl ion with a Si(CH3)3 molecule, giving off ammonia.  This gives an
inorganic/organic molecule, bonded to the wafer.   The Three (CH3) atoms are on
the surface and there is not a chemical bond between the resist and the methyl
but the resist intertwines with the organic Methyl's for better adhesion.  So
you get a great bond at the wafer surface and a good interaction at the resist
face.  Experiments show a reduction in roughness of the resist/wafer Critical
Dimension from 0.8 microns +/- 10% down to 0.8 microns +/- 4%.  The 4% is the
roughness of the original resist line seen at the developed image.  If the
developed image can be improved the roughness o
 f
>  the finished line can be improved.  Bill
>
>
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk



--
-Nathan
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply